°ÇÁ¶
¾ÐÃ⼺Çü
»çÃ⼺Çü
¾ÐÃâºí·ÎÀ×
¼öºÐÀ» Èí¼öÇÏ´Â ¼ºÁúÀÌ ÀÖ¾î, ÀÌ ¼ºÁú¿¡ ÀÇÇÏ¿© °¡°ø Áß ¼öºÐ¿¡ ÀÇÇÏ¿© ¹°¼ºÀúÇϰ¡ ÀÏ¾î ³¯ ¼ö ÀÖ½À´Ï´Ù. ÀÌ·¯ÇÑ ¹°¼º ÀúÇϸ¦ ¹æÁöÇϱâ À§ÇÏ¿©, °¡°ø Àü¿¡ ÃæºÐÇÑ °ÇÁ¶¸¦ ÇÊ¿ä·Î ÇÕ´Ï´Ù.
°ÇÁ¶¿Âµµ
65¡É (149¢µ)
°ÇÁ¶½Ã°£
Min.6 Hours / Max.12 Hours
°ÇÁ¶°ø±â À¯ÀÔ·®
> 0.065 §©/min per kg/hr (1cfm per lb/hr)
³ëÁ¡¿Âµµ
< -30¡É, -40¡É is better for good drying
¼öºÐÇÔ·®
< 0.05% (500ppm)
°ÇÁ¶±â ¿ë·®
6-12 times extruder output
°ÇÁ¶±â ³ôÀÌ/Æø ºñÀ²
> 2:1, 3:1 is better for plug flow of materials
´Ü¿
Insulate well to improve the efficiency
¸ð´ÏÅ͸µ
Inlet Air Temperature & Drew Point
PolymerÀÇ ºÐÀÚ·® °¨¼Ò¿¡ ÀÇÇÑ Á¦Ç° ¹°¼º ÀúÇÏ
ÃÖÁ¾ Á¦Ç°ÀÇ Color ºÒ·®
Á¦Ç° °¡°ø¼º»óÀÇ ¹®Á¦ ¹ß»ý
Á¦Ç° ¿Ü°ü ºÒ·®¹ß»ý